Feature

Aircraft Engine Blade Process Groove CNC Polishing: Process Optimization for Improved Vibration Fatigue Performance

FAQ

We work with a wide range of materials including aluminum, stainless steel, brass, copper, titanium, plastics (e.g., POM, ABS, PTFE), and specialty alloys. If you have specific material requirements, our team can advise the best option for your application.

Our CNC machining services cater to a variety of industries including aerospace, automotive, medical, electronics, robotics, and industrial equipment manufacturing. We also support rapid prototyping and custom low-volume production.

We typically achieve tolerances of ±0.005 mm (±0.0002 inches) depending on the part geometry and material. For tighter tolerances, please provide detailed drawings or consult our engineering team.

Standard lead times range from 3 to 10 business days, depending on part complexity, quantity, and material availability. Expedited production is available upon request.

Can you provide custom CNC prototypes and low-volume production?

Hot Posts

Insufficient vibration fatigue life in aircraft engine compressor blades results from machining defects in process grooves.

This study investigates CNC polishing technology for narrow machining grooves on aircraft engine blades.

It analyzes the machining process systematically. It also aims to optimize process groove machining and improve blade quality.

High-precision, fine-grained, super-hard abrasive electroplated diamond polishing wheels were used as processing tools, with synthetic diamond as the core abrasive.

At the same time, high-precision CNC polishing machines were used for polishing, and high-magnification electronic microscopes were employed to inspect the surface quality and shape of the process slots.

Failure Analysis

  • Macroscopic Observation

After vibration fatigue testing of the compressor straightening blades, cracks appeared at the root of the blade body, specifically at the radius (R) of the root corner.

Cracks initiated at a notch close to the radius (R) and extended laterally along the blade root. Figure 1 marks the position of this notch.

We opened the cracks to observe their fracture surfaces. Both blades shared identical fracture surface features: their cross-sections remained mostly flat and displayed distinct fatigue arc marks.

Figure 2 shows that the crack initiated from a point source at the interface between the notched blade cup side and the blade body surface.

Fig 1 Morphology characteristics of blade cracks and notches
Fig 1 Morphology characteristics of blade cracks and notches
Fig 2 Fracture morphology characteristics corresponding to fatigue cracks
Fig 2 Fracture morphology characteristics corresponding to fatigue cracks
  • Electron Microscopy Examination

Scanning electron microscope observations examine blade fracture surfaces. No material defects appear in the root zones of either blade sample. Distinct fatigue arcs and subtle fatigue bands emerge within crack propagation zones.

The artificially induced fracture region shows ductile dimple features, as displayed in Figures 3 and 4.

Fig 3 SEM morphology characteristics of fracture surface of blade No1
Fig 3 SEM morphology characteristics of fracture surface of blade No1
Fig 4 SEM morphology characteristics of fracture surface of blade No2
Fig 4 SEM morphology characteristics of fracture surface of blade No2
  • Comprehensive Analysis

The test results indicate that the cracks in the blade are fatigue cracks, with the origin located at the transition between the side notch of the blade cup and the blade body surface.

In blade vibration fatigue tests, under normal conditions, the position adjacent to the corner R in the middle of the blade’s back surface is where stress is highest;

Theoretically, fatigue cracks often initiate in this region.

However, there is a notch near the corner R on the blade body, which creates conditions for high stress concentration during vibration fatigue testing, making it more prone to fatigue crack initiation.

We therefore conclude that high stress concentration at the notch in the source region primarily triggers fatigue crack initiation.

Machining Improvements

  • Causes of Defects

Figure 5 marks the process groove at the junction of the blade tip and the cylindrical section. Turning first forms this groove, yet turning yields poor surface quality. We therefore grind this region.

However, this area is extremely small (R1 semicircular arc), making manual polishing impossible. We first adopted manual grinding and used a cylindrical oilstone to machine the surface of the process groove.

Fig 5 Position of the process groove
Fig 5 Position of the process groove

Manual grinding is prone to variations due to differences in worker experience;

Furthermore, because the work area is too narrow, it is difficult to control the grinding path and pressure.

As a result, the machined grooves are prone to sharp edges, notches, and excessively sharp arcs, as shown in Figure 6.

Fig 6 Sharp edge notch
Fig 6 Sharp edge notch

Furthermore, the manual grinding process involves low-speed, low-overlap reciprocating grinding, which cannot achieve a high surface finish;

Therefore, the surface finish of the ground blades is poor, as shown in Figure 7.

Fig 7 Surface quality of the process groove
Fig 7 Surface quality of the process groove
  • Optimization Analysis

Other scholars put forward this core idea. Manufacturing fatigue-resistant, long-life components covers two key stages.

The first stage blocks crack initiation sources. The second stage slows crack propagation. Targeted process adjustments improve the work-hardened layer systematically.

These adjustments optimize its microstructure, micromechanical response and surface integrity. Surface defects and microcracks propagate more slowly. The component gains a longer crack initiation life.

Surface integrity includes eight core technical dimensions. They are surface roughness, residual stress field, work hardening effect, surface geometry, subsurface defects, subsurface metallographic structure, edge forming quality, and other special surface attributes.

Process grooves and blade tip structures depend on four critical factors. These factors are surface roughness, surface topography, surface defects, and edge quality.

They dominate the vibration fatigue performance of these regions. This study follows the scheme proposed by Zhang Xifang et al.

The scheme optimizes machining parameters and uses sharp cutting tools. It selects suitable lubrication approaches.

High-rigidity, high-precision and vibrationfree machine tools work together. These measures deliver reliable control of final surface quality.

Blades feature complex surfaces, low rigidity and hard-to-machine material properties. Figure 8 lists mainstream mechanical machining methods for controlling surface integrity.

The CNC polishing technology adopted in this study belongs to high-efficiency precision grinding. CNC polishing machines run at high speed with high precision and low vibration. Diamond polishing wheels provide high precision and a broad selection of grit sizes.

When used in conjunction with cutting fluid, this process can significantly improve the surface quality of the process grooves and blade tips, thereby markedly enhancing vibration fatigue performance.

Fig 8 Machining technology for blade surface integrity
Fig 8 Machining technology for blade surface integrity
  • CNC Polishing Tools and Equipment

1. Limitations of Commercially Available Polishing Tools

Traditional polishing tools on the market have several common forms. They include straight polishing wheels, louvered wheels and rubber polishing wheels.

Resin polishing wheels and scouring pad polishing wheels are also widely used. One type mixes abrasives and plastics into brush-shaped or filament-structured wheels.

Other tools combine wool wheels, cloth wheels or wire wheels with fluid abrasives. Blade process grooves impose strict technical constraints. For the R1.0 mm small-radius arc, the polishing tool radius must not exceed R1.0 mm.

Abrasives also need strong bonding resistance against detachment. Small-radius polishing tools deform easily under compression and wear quickly.

Their substrate must retain adequate rigidity. This rigidity gives abrasives proper elasticity and contact pressure.

Groove CNC polishing demands polishing wheels with stable geometry and good wear resistance. Otherwise, we cannot guarantee consistent surface quality.

In summary, commercially available radius polishing tools are unable to meet the high-precision machining requirements for process channels.

2. Design and Structure of the Improved Elastic Polishing Wheel

This research adopts the elastic polishing wheel with a locally reinforced structure from Chen Zhitong et al. and Zhou Zhengmin et al.

It references the process schemes of DYNATICS and Xiao G. A conventional polishing wheel serves as the base substrate.

We add reinforcement structures or fillers between the abrasives and the elastic matrix.

This design strengthens abrasive bonding. It achieves precise control of local supporting structures and enables small-radius polishing tool fabrication.

Traditional polishing wheels suffer several technical drawbacks. Their contour and geometric surface change abruptly. Abrasives hold weakly, sink into the substrate, and fall off prematurely.

Material removal lacks stable performance. This work develops a systematic solution for these problems.

We control the working-end fillet radius of the polishing wheel within the range of R0.9 mm to R0.95 mm. This value is slightly smaller than the target R1.0 mm groove bottom.

A tiny polishing allowance remains to avoid rigid interference between the wheel and groove wall.

We corrected dynamic measurement deviations with an equivalent diameter model and improved the accuracy by 2.02%.

This ensures uniform contact area for the wheel within the narrow groove and eliminates contact blind spots at the groove bottom and root corners.

A photograph of the polishing wheel is shown in Figure 9.

Fig 9 Flexible diamond polishing wheel
Fig 9 Flexible diamond polishing wheel

3. Selection of Abrasive Grit and Polishing Equipment Parameters

The polishing wheel with 1200# grit suits the machining needs of process grooves and delivers acceptable service life.

It controls material removal volume accurately inside grooves. The surface roughness stably stays within Ra 0.2–0.5 μm.

This performance satisfies the high-precision polishing requirements for precision components.

Therefore, a 1,200# diamond polishing wheel is used for rough polishing and deburring of the process channel and blade tips.

The 2000-grit polishing wheel features finer abrasives and achieves a lower material removal rate. The 2000-grit diamond polishing wheel upgrades surface quality.

It avoids over-polishing on groove walls and fillet deformation at the root of narrow process grooves.

We select an eight-axis, six-axis-interpolated polishing machine as the CNC polishing equipment; its spindle speed ranges from 300 to 30,000 r/min.

Positioning accuracy: X, Y, Z ≤ 0.008 mm; B-axis ≤ 20″; C-axis ≤ 60″; Repeatability: X, Y, Z ≤ 0.005 mm; B-axis ≤ 15″; C-axis ≤ 40″.

Feed rates: Rapid feed on the X, Y, and Z axes ≥9 m/min; cutting feed 1–5,000 mm/min;

B-axis feed 0–10 r/min; C-axis feed 0–20 r/min. Capable of performing CNC polishing of surfaces and curved edges in machining slots.

  • CNC Polishing Technology for Process Tanks and Establishment of a Coordinate System

1. Tool Setting and Positioning Scheme of the CNC Polishing System

We encounter tool-setting issues when polishing on the eight-axis, six-axis-linked CNC polishing machine.

For this reason, after we mount the diamond polishing wheel onto the spindle, we determine the relative positional relationship between the polishing wheel and the slide.

A platform-based dial gauge method is used to determine the position of the workpiece on the machine’s X-axis (as shown in Figure 10), driving the workpiece to complete the longitudinal feed movement.

The upper cone serves as the positioning datum for the long shaft neck end of the blade.

We need to confirm the spatial relation between the chuck and this upper cone (Figures 11–12) and check for potential interference.

A positioning sleeve is custom-made for alignment against the conical datum. Its positional error stays within ±0.01 mm.

The tool spindle tilts by 15°–20° relative to the normal of the groove bottom surface. This tilt avoids collisions between the polishing wheel spindle and groove side walls.

Meanwhile, the effective abrasive working surface fully covers the R1.0 mm arc profile of the groove.

2. Workpiece Clamping and Coordinate System Establishment

Clamp the two journal ends of the blade onto the A+ and A- chucks for automatic centering, enabling rotational adjustment of the workpiece.

A special sleeve ensures that the circular platform and the chucks remain fixed in position.

The machining coordinate system is based on the machine tool’s A-axis, which drives the blade workpiece to rotate around the X-axis, adjusting the polishing orientation of the blade surface.

The A-axis rotation center serves as the origin of the machine tool coordinate system for the A-axis.

We select the fifth cross-section of the blade body to rigidly support the workpiece and compensate for tool wear.

The spindle head performs auxiliary positioning, clamping and alignment tasks. This setup keeps the workpiece at the target A-axis angle as it rotates about the X-axis.

2. Dynamic Preload Compensation Mechanism

This study builds a dynamic preload compensation mechanism. Once the polishing wheel wears, the system adjusts the preload continuously and automatically in real time.

This compensates for falling contact pressure induced by abrasive wear. Polishing force fluctuates within ±0.5 N during the whole process.

Material removal depth remains uniform along the full length of the R1.0 mm groove. The clamping and positioning are shown in Figure 13.

Fig 10 X axis calibration of the workpiece to be machined
Fig 10 X axis calibration of the workpiece to be machined
Fig 11 Positioning of the spindle and the workpiece
Fig 11 Positioning of the spindle and the workpiece
Fig 12 Positioning of the chuck and the upper circular platform
Fig 12 Positioning of the chuck and the upper circular platform
Fig 13 Clamping and positioning
Fig 13 Clamping and positioning
  • Machining Procedure

Figure 14 illustrates the machining positions on the blade. We carry out CNC polishing at position A, along all sharp edges D, and on the blade tip surface.

Fig 14 Schematic diagram of blade machining position
Fig 14 Schematic diagram of blade machining position

We divide the tool path into six steps following the principle: rough machining adopts high feed rates for high efficiency, while finish machining uses low feed rates to guarantee precision.

Rough polishing of the blade tip’s sharp edges → Rough polishing of the process groove arcs → Rough polishing of the blade tip’s long edges → Fine polishing of the blade tip’s sharp edges → Fine polishing of the process groove arcs → Fine polishing of the blade tip’s long edges.

1. Rough Polishing of Blade Tip Sharp Edges

Polish the sharp edges of the blade tip to create a fillet of R0.2–R0.6 mm and remove turning marks. We adjust and optimize the parameters to achieve both cost-effectiveness and high efficiency.

Figure 15 presents the machining parameters, which we summarize in Table 1.

Fig 15 Rough polishing of blade tip sharp edge
Fig 15 Rough polishing of blade tip sharp edge
ParameterValue
Polishing wheel grit size1200#
Rotational speed (r/min)1,500
Feed rate (mm/min)800
Pre-compression amount (mm)0.2
ModelD20R1.0

Table 1. Parameters of Rough Polishing for the Blade Tip Sharp Edge

2. Rough Polishing of the Process Groove Arc

Perform rough polishing on the arc of the process groove at the blade tip. The working surface of the polishing wheel aligns with the process groove, mirroring the shape of a semicircular arc.

At a speed of 2,000 rpm, it can easily remove turning tool marks from within the process groove and produce a good surface finish.

In addition, adjust the angle of the spindle so that the cutting edge of the polishing wheel completely covers the machining groove.

As shown in Figure 16, the machining parameters are listed in Table 2.

Fig 16 Rough polishing of process groove arc
Fig 16 Rough polishing of process groove arc
ParameterValue
Polishing wheel grit size1200#
Rotational speed (r/min)2,000
Feed rate (mm/min)800
Pre-compression amount (mm)0.2–0.3
ModelD20R1.0

Table 2. Parameters of Rough Polishing for the Process Groove Arc

3. Rough Grinding of the Long Edge of the Blade Tip

Perform rough grinding on the flat surface of the long edge of the blade tip to improve grinding efficiency and quickly level the blade tip surface, as shown in Figure 17.

The machining parameters are listed in Table 3.

Fig 17 Rough polishing of blade tip long edge
Fig 17 Rough polishing of blade tip long edge
ParameterValue
Polishing wheel grit size1200#
Rotational speed (r/min)2,000
Feed rate (mm/min)3,000
Pre-compression amount (mm)0.2–0.3
ModelD20R1.0

Table 3. Parameters of Rough Polishing for the Blade Tip Long Edge

4. Fine Polishing of the Sharp Edges at the Blade Tips

After rough polishing, the shape of the process groove and the blade tips has been formed, but the surface roughness is poor, so a polishing wheel with a finer grit must be used for fine polishing.

Therefore, a 2,000-grit polishing wheel was installed, the feed rate was reduced, and the rotational speed was increased to perform fine polishing on the sharp edges of the blade tips, thereby improving surface roughness and ensuring smooth transitions.

The pre-pressure was reduced to 0.05–0.10 mm to achieve only nanometer-level material removal, thereby completing the mirror-finish polishing of the groove surface without damaging the machined contour.

As shown in Figure 18, the machining parameters are listed in Table 4.

Fig 18 Finish polishing of blade tip sharp edge
Fig 18 Finish polishing of blade tip sharp edge
ParameterValue
Polishing wheel grit size2000#
Rotational speed (r/min)5,000
Feed rate (mm/min)400
Pre-compression amount (mm)0.1
ModelD20R1.0

Table 4. Parameters of Finish Polishing for the Blade Tip Sharp Edge

5. Precision Polishing of the Process Groove Arc

Perform precision polishing on the arc of the process groove at the blade tip; The working surface of the polishing wheel aligns with the process groove, mirroring the shape of a semicircular arc.

At a rotational speed of 3,000 rpm, this further improves the surface roughness. As shown in Figure 19, the machining parameters are listed in Table 5.

Fig 19 Finish polishing of process groove arc
Fig 19 Finish polishing of process groove arc
ParameterValue
Polishing wheel grit size2000#
Rotational speed (r/min)3,000
Feed rate (mm/min)400
Pre-compression amount (mm)0.1
ModelD25R1.0

Table 5. Parameters of Finish Polishing for the Process Groove Arc

6. Fine Polishing of the Long Edge of the Blade Tip

Fine polishing treats the flat surface on the long edge of the blade tip. It removes fine, dense grinding marks left from rough polishing.

The treatment optimizes surface texture and reduces surface roughness. Table 6 records the corresponding machining parameters, as illustrated in Figure 20.

CNC polishing is performed on the process grooves and blade tips of compressor straightening blades.

After rough polishing to shape and fine polishing to enhance the finish, the surface roughness, surface morphology, edge quality were significantly improved, and surface defects were greatly reduced.

The blades were inspected before and after polishing using an electronic magnifying glass, as shown in Figure 21.

Fig 20 Finish polishing of blade tip long edge
Fig 20 Finish polishing of blade tip long edge
Fig 21 Quality inspection of CNC polishing
Fig 21 Quality inspection of CNC polishing
ParameterValue
Polishing wheel grit size2000#
Rotational speed (r/min)5,000
Feed rate (mm/min)1,000
Pre-compression amount (mm)0.1
ModelD20R1.0

Table 6. Parameters of Finish Polishing for the Blade Tip Long Edge

Test Results

  • Surface Roughness

Before Improvement: After manual grinding of a narrow 1.0 mm process groove, the initial roughness was Ra 1.6–6.3 μm, with noticeable tool marks and a machined layer remaining on the surface.

After Improvement: Following semi-finishing with a 1,200-grit polishing wheel, the roughness stabilized at Ra 0.2–0.5 μm, completely removing the original deep tool marks, with no visible macro-scratches on the surface.

After fine polishing with a 2,000-grit polishing wheel, the final surface roughness can reach Ra 0.05–0.15 μm.

For materials commonly used in the aerospace industry, such as titanium alloys, the surface roughness can be consistently controlled within the Ra 0.05–0.15 μm range, achieving a near-mirror finish.

  • Groove Profile and Arc Radius

Before Improvement: After milling, the groove profile error was approximately ±0.03 mm, the deviation in the R1.0 mm arc radius was ±0.05 mm, and there was noticeable chipping at the corner positions.

After Improvement: Through precise control of the cutting path and preload, the overall groove profile error is ≤±0.01 mm, and the R1.0 mm arc radius error is stably controlled within ±0.02 mm.

There is no corner distortion caused by over-polishing, and the original design profile reference is fully preserved.

  • Fatigue Test Results

One batch of blades was selected for CNC polishing. After passing the inspection, fatigue testing was conducted, and the results are as follows:

Under the specified maximum stress and cycle count requirements, all blades passed the fatigue test (as shown in Table 7).

Batch Number and Data PointStress (MPa)Fatigue Test Result
Blade No.StatusPoint No. 1Pass
Blade 1Finished product awaiting delivery-417Pass
Blade 2Finished product awaiting delivery-424Pass
Blade 3Finished product awaiting delivery-384Pass
Blade 4Finished product awaiting delivery-503Pass
Blade 5Finished product awaiting delivery-774Pass
Blade 6Finished product awaiting delivery-229Pass
Blade 7Finished product awaiting delivery-597Pass
Blade 8Finished product awaiting delivery-675Pass
Blade 9Finished product awaiting delivery-334Pass
Blade 10Finished product awaiting delivery-235Pass
Blade 11Finished product awaiting delivery-468Pass
Blade 12Finished product awaiting delivery-551Pass

Table 7. Fatigue Test Results

Upon inspection, the blade surfaces were found to be intact, with no defects or cracks.

This result demonstrates that CNC polishing with flexible diamond polishing wheels works well for blade process grooves.

It eliminates notches near the R-corner that arise from manual polishing. Crack initiation at the root gets suppressed during vibration fatigue tests. Both the machining quality and processing efficiency of blades improve accordingly.

Conclusion

  • Point One

The developed CNC polishing process for narrow process grooves can effectively eliminate defects resulting from initial machining, achieving dual optimization of the surface quality and contour accuracy of the process grooves.

Test results verify the performance of this process. It cuts the initial Ra of process grooves from 1.6–6.3 μm down to 0.05–0.15 μm.

The radius error of the R1.0 mm groove-bottom arc shrinks from ±0.05 mm to within ±0.02 mm. The machined profile faithfully reproduces the smooth contour of the design datum.

Stress distortion induced by abrupt geometric variation in the groove region disappears. This approach blocks fatigue defect initiation at its machining source.

  • Second Point

Smoothing the surface profile of the machining grooves can significantly reduce the level of local stress concentration.

Unpolished process grooves create a high-risk condition. Sharp corners and micro-notches at groove roots produce stress concentration factors 5–10 times the nominal stress.

This serves as a major driver of blade fatigue fracture. Optimized polishing generates a continuous, smooth profile. Stress spreads evenly under airflow and cyclic mechanical loads.

Local peak stress in the groove region drops by over 60%. Abnormal stress concentration originating from microscopic machining defects gets fundamentally avoided.

  • Third Point

Improvements in the polishing quality of the process groove directly translate into quantifiable gains in the blade’s resistance to vibration-induced fatigue.

Blades polished by this process passed the full-condition vibration fatigue test on the first trial. They completed the required loading cycles at a maximum stress of −774 MPa.

The design specification sets the blade vibration fatigue limit σ₋₁ at −641 MPa. Vibration fatigue resistance increased by 20.69%.

This outcome directly solves an engineering problem. Earlier production batches repeatedly failed vibration fatigue tests.

The process offers practical engineering guidance for high-precision polishing and fatigue-oriented manufacturing of narrow complex grooves on similar aero-engine components.

The future of manufacturing will move toward automation, intelligent, and information-based manufacturing, and this research on CNC polishing technology has laid a solid foundation for the comprehensive advancement of digital manufacturing in the aerospace industry.

It also provides technical support for the subsequent establishment of automated, intelligent, and information-based manufacturing systems.

Table of Contents

Let's Start A New Project Today